Chemical composition [% max. or range]

SiFeCuMnMgCrNiZnTiGaV
0,30,50,050,150,7–1,10,10,2

Heat-treated condition 0/H111 | EN AW 5005A

Mechanical properties

Nominal thickness
mm
Brinell hardness
HBW
Yield strength
Rp0,2 MPa
min./max.
Tensile strength
Rm MPa
min./max.
Elongation
A50
mm %
min.
Elongation
A %
min.
Bending radius
180° t
min.
Bending radius
90° t
min.
0,2 - 0,52935100 - 145150 t0 t
0,5 - 1,52935100 - 145190 t0 t
1,5 - 32935100 - 145200,5 t0 t
3 - 62935100 - 145221,0 t1,0 t
6 - 12,52935100 - 145241,5 t
12,5 - 502935100 - 14520

Heat-treated condition H14 | EN AW 5005A

Mechanical properties

Nominal thickness
mm
Brinell hardness
HBW
Yield strength
Rp0,2 MPa
min./max.
Tensile strength
Rm MPa
min./max.
Elongation
A50
mm %
min.
Elongation
A %
min.
Bending radius
180° t
min.
Bending radius
90° t
min.
0,2 - 0,548120145 - 18522,0 t0,5 t
0,5 - 1,548120145 - 18522,0 t1,0 t
1,5 - 348120145 - 18532,5 t1,0 t
3 - 648120145 - 18542,0 t
6 - 12,548120145 - 18552,5 t

Heat-treated condition H22 | EN AW 5005A

Mechanical properties

Nominal thickness
mm
Brinell hardness
HBW
Yield strength
Rp0,2 MPa
min./max.
Tensile strength
Rm MPa
min./max.
Elongation
A50
mm %
min.
Elongation
A %
min.
Bending radius
180° t
min.
Bending radius
90° t
min.
0,2 - 0,53880125 - 16541,0 t0 t
0,5 - 1,53880125 - 16551,0 t0,5 t
1,5 - 33880125 - 16561,5 t1,0 t
3 - 63880125 - 16581,0 t
6 - 12,53880125 - 165102,0 t

Heat-treated condition H24 | EN AW 5005A

Mechanical properties

Nominal thickness
mm
Brinell hardness
HBW
Yield strength
Rp0,2 MPa
min./max.
Tensile strength
Rm MPa
min./max.
Elongation
A50
mm %
min.
Elongation
A %
min.
Bending radius
180° t
min.
Bending radius
90° t
min.
0,2 - 0,547110145 - 18531,5 t0,5 t
0,5 - 1,547110145 - 18541,5 t1,0 t
1,5 - 347110145 - 18552,0 t1,0 t
3 - 647110145 - 18562,0 t
6 - 12,547110145 - 18582,5 t

Heat-treated condition H26 | EN AW 5005A

Mechanical properties

Nominal thickness
mm
Brinell hardness
HBW
Yield strength
Rp0,2 MPa
min./max.
Tensile strength
Rm MPa
min./max.
Elongation
A50
mm %
min.
Elongation
A %
min.
Bending radius
180° t
min.
Bending radius
90° t
min.
0,2 - 0,552135165 - 20521,0 t
0,5 - 1,552135165 - 20531,5 t
1,5 - 352135165 - 20542,0 t
3 - 452135165 - 20542,5 t

Heat-treated condition H28 | EN AW 5005A

Mechanical properties

Nominal thickness
mm
Brinell hardness
HBW
Yield strength
Rp0,2 MPa
min./max.
Tensile strength
Rm MPa
min./max.
Elongation
A50
mm %
min.
Elongation
A %
min.
Bending radius
180° t
min.
Bending radius
90° t
min.
0,2 - 0,55816018511,5 t
0,5 - 1,55816018522,5 t
1,5 - 35816018533,0 t