EN AW 3004 | Al Mn1Mg1
On this page you can find the chemical and mechanical specifications of the alloy EN AW 3004 | Al Mn1Mg1.
Other dimensions and alloys are available on request.
Our aluminum specialists in Mannheim are happy to advise you. EN AW 3004 - send request!
Chemical composition [% max. or range]
Si | Fe | Cu | Mn | Mg | Cr | Ni | Zn | Ti | Ga | V |
0.3 | 0.7 | 0.25 | 1.0–1.5 | 0.8–1.3 | — | — | 0.25 | — | — | — |
EN AW 3004 | Al Mn1Mg1: Heat-treated condition 0/H111
Mechanical properties
Nominal thickness mm | Brinell hardness HBW | Yield strength Rp0,2 MPa min./max. | Tensile strength Rm MPa min./max. | Elongation A50 mm % min. | Elongation A % min. | Bending radius 180° t min. | Bending radius 90° t min. |
0.2 - 0.5 | 45 | 60 | 155 - 200 | 13 | 0 t | 0 t | |
0.5 - 1.5 | 45 | 60 | 155 - 200 | 14 | 0 t | 0 t | |
1.5 - 3 | 45 | 60 | 155 - 200 | 15 | 0.5 t | 0 t | |
3 - 6 | 45 | 60 | 155 - 200 | 16 | 1.0 t | 1.0 t | |
6 - 12.5 | 45 | 60 | 155 - 200 | 16 | 2.0 t | ||
12.5 - 50 | 45 | 60 | 155 - 200 | 14 |
EN AW 3004 | Al Mn1Mg1: Heat-treated condition H22
Mechanical properties
Nominal thickness mm | Brinell hardness HBW | Yield strength Rp0,2 MPa min./max. | Tensile strength Rm MPa min./max. | Elongation A50 mm % min. | Elongation A % min. | Bending radius 180° t min. | Bending radius 90° t min. |
0.2 - 0.5 | 58 | 145 | 190 - 240 | 4 | 1.0 t | 0 t | |
0.5 - 1.5 | 58 | 145 | 190 - 240 | 5 | 1.0 t | 0.5 t | |
1.5 - 3 | 58 | 145 | 190 - 240 | 6 | 1.5 t | 1.0 t | |
3 - 6 | 58 | 145 | 190 - 240 | 7 | 1.5 t |
EN AW 3004 | Al Mn1Mg1: Heat-treated condition H24
Mechanical properties
Nominal thickness mm | Brinell hardness HBW | Yield strength Rp0,2 MPa min./max. | Tensile strength Rm MPa min./max. | Elongation A50 mm % min. | Elongation A % min. | Bending radius 180° t min. | Bending radius 90° t min. |
0.2 - 0.5 | 66 | 170 | 220 - 265 | 3 | 2.0 t | 0.5 t | |
0.5 - 1.5 | 66 | 170 | 220 - 265 | 4 | 2.0 t | 1.0 t | |