EN AW 7020 | Al Zn4.5Mg1
Chemical composition [% max. or range]
Si | Fe | Cu | Mn | Mg | Cr | Ni | Zn | Ti | Ga | V |
0.35 | 0.4 | 0.2 | 0.05–0.50 | 1.0–1.4 | 0.10–0.35 | — | 4.0–5.0 | — | — | — |
Heat-treated condition T4 | EN AW 7020
Mechanical properties
Nominal thickness mm | Brinell hardness HBW | Yield strength Rp0,2 MPa min./max. | Tensile strength Rm MPa min./max. | Elongation A50 mm % min. | Elongation A % min. | Bending radius 180° t min. | Bending radius 90° t min. |
>= 0.4 - 1.5 | 92 | 210 | 320 | 11 | 2.0 t | ||
1.5 - 3 | 92 | 210 | 320 | 12 | 2.5 t | ||
3 - 6 | 92 | 210 | 320 | 13 | 3.5 t | ||
6 - 12.5 | 92 | 210 | 320 | 14 | 5.0 t |
Heat-treated condition T6 | EN AW 7020
Mechanical properties
Nominal thickness mm | Brinell hardness HBW | Yield strength Rp0,2 MPa min./max. | Tensile strength Rm MPa min./max. | Elongation A50 mm % min. | Elongation A % min. | Bending radius 180° t min. | Bending radius 90° t min. |
>= 0.4 - 1.5 | 104 | 280 | 350 | 7 | 3.5 t | ||
1.5 - 3 | 104 | 280 | 350 | 8 | 4.0 t | ||
3 - 6 | 104 | 280 | 350 | 10 | 5.5 t | ||
6 - 12.5 | 104 | 280 | 350 | 10 | 8.0 t | ||
12.5 - 40 | 104 | 280 | 350 | 9 | |||
40 - 100 | 101 | 270 | 340 | 8 | |||
100 - 150 | 98 | 260 | 330 | 7 | |||
150 - 175 | 98 | 260 | 330 | 6 | |||
175 - 250 | 260 | 330 | 5 |